Title:
Reverse flotation of iron ore using purified cotton seed fattyacid at ambient temperature
文章编号:
1674-2869(2015)12-0036-05
作者:
魏以和1魏建勋 1郭文达 1周高云2
1.武汉工程大学资源与土木工程学院,湖北武汉430074;2. 北京矿冶研究总院,北京102600
Author(s):
WEI Yi-he1WEI Jian-xun1GUO Wen-da1ZHOU Gao-yun2
1. School of Resource and Civil Engineering,Wuhan Institute of Technology, Wuhan 430074,China 2. Beijing General Research Institute of Mining & Metallurgy,Beijing 102600,China
关键词:
棉籽油酸常温反浮选 磁铁精矿尿素包裹法阴离子捕收剂
Keywords:
cottonseed fatty acid reverse flotation at ambient temperature magnetic concentrateurea adduct method anionic collector
分类号:
TD923
DOI:
10. 3969/j. issn. 1674-2869. 2015. 12. 008
文献标志码:
A
摘要:
为了解决铁矿石阴离子加温反浮选的高能耗问题,利用尿素包裹法分离纯化的棉籽油酸复配的捕收剂进行了常温(15 ℃)反浮选试验. 以齐大山铁矿磁铁精矿为反浮选研究对象, 确定了最佳药剂耗量为:粗选氢氧化钠 0.7 kg/t、淀粉0.4 kg/t、氯化钙0.1 kg/t、捕收剂0.4 kg/t、扫选淀粉0.2 kg/t.开路获得铁精矿品位63.64%、回收率47.88%,并经过闭路试验得到铁精矿品位63.75%、回收率 89.47%的选矿指标. 试验表明纯化后的棉籽油酸常温捕收能力增强,复配16.7%阴离子表面活性剂后捕收能力进一步增强. 为解决常规加温反浮选能耗大,成本高的问题提供了一条可能的途径.
Abstract:
To solve the problem of high energy consumption in heated reverse flotation of iron?鄄ore, flotation tests with purified cotton seed fatty acid by urea adduct method were conducted under normal conditions (15 ℃). Aimed at the reverse flotation of the magnetic concentrate of Qidashan iron ore, the optimum reagent consumption, sodium hydroxide of 0.7 kg/t, starch of 0.4 kg/t, calcium chloride of 0.1 kg/t, collector of 0.4 kg/t, and scavenging starch of 0.2 kg/t ,were gotten. The grade of iron concentrate of 63.64% and recovery rate of 47.88% were obtained in open circuit test. The grade of iron concentrate of 63.55% and recovery rate of 89.47% were obtained in closed circuit test. The test results show that the collecting capacity of purified cotton seed fatty acid under normal conditions is strengthened, which is further enhanced after mixed with an anionic surfactant of 16.7%. It provides a potential way for solving the problem of high energy consumption and high cost in conventional heated reverse flotation.

参考文献/References:

[1]  李维兵,宋仁峰,刘华艳.我国难选铁矿石选矿技术进步评述[J].金属矿山,2008,38(11) :1-4.LI Wei-bing, SONG Ren-feng, LIU Hua-yan. Review of China's progress in beneficiation technology for refractory iron ores[J]. Metal Mine, 2008,38(11): 1-4.(in Chinese)[2] 张朝宏,戴惠新.铁矿石反浮选捕收剂现状及未来发展趋势[J].矿产综合利用,2012(4):3-6.ZHANG Chao-hong, DAI Hui-xin. Current situation and future development of the collector for reverse flotation of iron ore[J]. Multipurpose Utilization of Mineral Resources, 2012(4):3-6.(in Chinese)[3] 朱玉霜,朱建光.浮选药剂的化学原理[M].长沙:中南工业大学出版社,1996: 60-68.ZHU Yu-shuang,ZHU Jian-guang. The chemical principle of flotation reagents[M].Changsha: Central South University of Technology Press,1996:60-68.(in Chinese)[4] 钟康年,罗惠华,姚杨.捕收剂的亚油酸/油酸比值对磷矿浮选的影响[J].化工矿物与加工,2003(11):1-3.ZHONG Kang-nian, LUO Hui-hua, YAO Yang. Effect of fatty acids with different ratio of linoleic acid/oleic acid on flotation of phosphate rock[J]. Industrial Minerals & Processing,2003(11):1-3.(in Chinese)[5] 罗惠华,汤家焰,李成秀,等. 胶磷矿选矿中不同植物脂肪酸的常温浮选性能[J]. 武汉工程大学学报, 2013, 35(1):17-20. LUO Hui-hua, TANG Jia-yan, LI Cheng-xiu, et al. Flotation performance of plant fatty acid on collophanite at normal temperature[J]. Journal of Wuhan Institute of Technology, 2013,35(1):17-20.(in Chinese)[6] 黄慧琴,鲍时翔.多价不饱和脂肪酸分离纯化技术进展[J].中国油脂,1999,24(2): 32-34.HUANG Hui-qin,BAO Shi-xiang. The separation and purification progress of multivalent unsaturated fatty acids[J]. China Oils and Fats,1999,24(2): 32-34.(in Chinese)[7] 张镜澄.超临界流体萃取[M].北京:化学工业出版社, 2000.ZHANG Jing-cheng. Super-critical extraction[M].Beijing: Chemical Industry Press,2000.(in Chinese)[8] Schilling P. Adhesion promoters for anionic bituminous emulsions: US, US 5667578 A [P]. 1997-09-16.[9] 纪军.高磷铁矿石脱磷技术研究[J],矿冶,2003(2):33-37.JI Jun. Study on dephosphorization technology for high-phosphorus iron ore[J],Mining & Metallurgy,2003(2):33-37.(in Chinese)[10] 张桂兰.含磷钒钛磁铁矿选铁试验[J].矿产综合利用,1996(2):22-25.ZHANG Gui-lan.Experimental research of iron concentration for a low grade vanadiferous titanomagnetite ore with high phosphorus[J]. Multipurpose Utilization of Mineral Resources,1996(2):22-25.(in Chinese)[11] 李丽匣,印万忠,冯丹,等.油酸钠体系下铁矿物及石英的浮选性能[J].金属矿山,2011(8):68-71.LI Li-xia, YIN Wan-zhong, FENG Dan,et al. Floatability performance of iron minerals and quartz in system of sodium oleate[J]. Metal Mine, 2011(8):68-71.(in Chinese)[12] 孙传尧,印万忠.硅酸盐浮选原理[M].北京:科学出版社,2001:126-127.SUN Chuan-yao,YIN Wan-zhong.The flotation principle of silicate[M].Beijing:Science Press,2001:126-127.(in Chinese)